17-4PH stainless steel is a martensitic precipitation-hardening stainless steel designed for applications that need high strength, useful corrosion resistance and controlled mechanical properties after aging. Common designations include UNS S17400, Type 630 / AISI 630, EN 1.4542 / X5CrNiCuNb16-4 and SUS630.
The alloy contains chromium, nickel, copper and niobium. After solution treatment, aging conditions such as H900, H925, H1025, H1075, H1100 and H1150 allow designers to trade maximum strength for greater ductility and toughness.
Compared with 304 stainless steel and 316L stainless steel, 17-4PH can achieve substantially higher strength after aging. Compared with 410 stainless steel and 420 stainless steel, it generally provides a more useful combination of strength, toughness and corrosion resistance.
What Is 17-4PH Stainless Steel?
17-4PH is a precipitation-hardening stainless steel that develops a martensitic structure after solution treatment and cooling. Copper-rich precipitation during aging increases strength and hardness without requiring the conventional quench-and-temper route used for many hardenable steels.
The designation “17-4” refers approximately to its chromium and nickel alloy concept, while “PH” means precipitation hardening. The grade is commonly used for shafts, valve parts, pump components, fasteners, aerospace fittings and other highly loaded machined parts.
High Strength
Aging can produce yield and tensile strength far above conventional annealed austenitic stainless steels.
Adjustable Properties
H900 through H1150 conditions provide different combinations of strength, hardness, ductility and toughness.
Useful Corrosion Resistance
Corrosion resistance is useful for many industrial environments while retaining much higher strength than common 300-series grades.
17-4PH Standards and Equivalent Designations
“17-4PH” alone is not enough for a critical purchase order. Buyers should specify the product form, governing material standard and required heat-treatment condition.
| System / Product Form | Designation or Specification | Procurement Meaning |
|---|---|---|
| UNS | S17400 | Primary UNS material designation. |
| AISI / Market | Type 630 / AISI 630 / 17-4PH | Common US and commercial grade names. |
| Europe | EN 1.4542 / X5CrNiCuNb16-4 | Common European material designation. |
| Japan | SUS630 | Common JIS grade reference. |
| Bar / Shape | ASTM A564/A564M | Age-hardening stainless steel bars and shapes. |
| Plate / Sheet / Strip | ASTM A693 | Precipitation-hardening stainless steel flat products. |
| Forging | ASTM A705/A705M | Age-hardening stainless steel forgings. |
| Aerospace Flat Product | AMS 5604 | Common aerospace specification for 17-4PH sheet, strip and plate. |
| Aerospace Bar / Forging | AMS 5643 | Common aerospace specification for wrought 17-4PH products. |
For additional grade cross-references, see the international steel grade equivalents chart and the stainless steel grades overview .
17-4PH Chemical Composition
The following chemistry is a practical reference for Type 630 / UNS S17400. Exact limits should be checked against the governing product specification and MTC.
| Element | Reference Limit | Role |
|---|---|---|
| Carbon (C) | ≤ 0.07% | Controlled to support toughness, weldability and heat-treatment response. |
| Chromium (Cr) | 15.00–17.50% | Primary element responsible for stainless corrosion resistance. |
| Nickel (Ni) | 3.00–5.00% | Supports toughness and transformation control. |
| Copper (Cu) | 3.00–5.00% | Provides the main precipitation-hardening response. |
| Niobium / Nb + Ta | 0.15–0.45% | Supports precipitation behavior and microstructural control. |
| Manganese (Mn) | ≤ 1.00% | Controlled steelmaking addition. |
| Silicon (Si) | ≤ 1.00% | Deoxidation and steelmaking control. |
| Phosphorus (P) | ≤ 0.040% | Controlled residual element. |
| Sulfur (S) | ≤ 0.030% | Controlled residual element affecting toughness and machinability. |
| Iron (Fe) | Balance | Base metal. |
Chemistry should be verified from the actual heat-number MTC. Aerospace, pressure, sour-service or other critical applications may require additional restrictions beyond the basic grade chemistry.
17-4PH Heat Treatment: H900 to H1150
17-4PH is commonly supplied in solution-treated Condition A and then aged to the required H condition. Lower aging temperatures generally produce higher strength and hardness. Higher aging temperatures generally reduce strength while improving ductility and toughness.
| Condition | Nominal Aging Temperature | Typical Time at Temperature | General Selection Direction |
|---|---|---|---|
| H900 | 482°C / 900°F | 1 hour | Highest common strength and hardness. |
| H925 | 496°C / 925°F | 4 hours | Very high strength with slightly more ductility than H900. |
| H1025 | 551–552°C / 1025°F | 4 hours | Balanced high strength and toughness. |
| H1075 | 580°C / 1075°F | 4 hours | Lower hardness with improved ductility. |
| H1100 | 593°C / 1100°F | 4 hours | Useful toughness and reduced residual stress. |
| H1150 | 621°C / 1150°F | 4 hours | Lower strength with greater ductility and toughness. |
Mechanical Properties of 17-4PH Stainless Steel
Mechanical properties depend strongly on heat-treatment condition, product form, section size, testing direction and applicable specification. The table below is therefore a selection reference rather than a universal acceptance table.
| Condition | Tensile Strength | 0.2% Yield Strength | Typical Hardness Direction |
|---|---|---|---|
| H900 | About 1310 MPa minimum reference level | About 1170 MPa minimum reference level | Approximately 40 HRC and above, depending on specification. |
| H925 | About 1170 MPa minimum reference level | About 1070 MPa minimum reference level | High hardness, below H900. |
| H1025 | About 1070 MPa minimum reference level | About 1000 MPa minimum reference level | Mid-30s HRC range is common. |
| H1075 | About 1000 MPa minimum reference level | About 860 MPa minimum reference level | Lower hardness with improved ductility. |
| H1100 | About 965 MPa minimum reference level | About 790 MPa minimum reference level | Lower hardness and higher toughness than H900. |
| H1150 | About 930 MPa minimum reference level | About 725 MPa minimum reference level | Generally the lowest hardness among these common single-aging conditions. |
Do not use these values as purchase-order acceptance criteria. ASTM A564, ASTM A693, ASTM A705, AMS specifications and customer drawings can use different requirements depending on product form and dimensions.
Physical Properties of 17-4PH Stainless Steel
| Property | Engineering Reference |
|---|---|
| Density | Approximately 7.75–7.80 g/cm³ |
| Elastic Modulus | Approximately 190–200 GPa at room temperature |
| Thermal Conductivity | Approximately 16–20 W/m·K depending on temperature and condition |
| Magnetic Response | Magnetic in common solution-treated and aged conditions |
| High-Strength Service Reference | Common wrought specifications reference service up to about 315°C / 600°F |
Physical-property data alone should not determine material selection. Strength retention, corrosion exposure, toughness, fatigue, stress level and heat-treatment condition should be considered together.
Corrosion Resistance, Welding and Machining
Corrosion Resistance
17-4PH provides useful corrosion resistance for a high-strength martensitic PH stainless steel and is used in atmospheric, industrial, food-processing, pump, valve and aerospace applications. It should not automatically be treated as a replacement for 316L in severe chloride exposure.
If chloride resistance is more important than very high heat-treated strength, compare the project requirement with 316L stainless steel or an appropriate 2205 duplex stainless steel grade.
Welding
17-4PH can be welded using qualified procedures. Fabrication is often performed before final aging so that the required mechanical properties can be developed after welding. Critical weldments should follow the applicable welding procedure, filler-metal requirement and post-weld heat-treatment specification.
Machining
Machining behavior depends strongly on condition. Solution-treated or overaged conditions are often easier to machine than high-hardness conditions. Final machining sequence should account for aging, dimensional tolerance and distortion control.
Typical Applications of 17-4PH Stainless Steel
Aerospace & Precision Engineering
Aircraft fittings, structural components, actuator parts, high-strength fasteners and precision machined components.
Pumps & Valves
Pump shafts, valve stems, sleeves, couplings, high-strength valve components and rotating parts.
Energy & Industrial Equipment
Shafts, fasteners, gears, mechanical hardware, process-equipment components and selected oil-and-gas parts.
Final suitability depends on loading, corrosion environment, service temperature, fatigue requirement, heat-treatment condition and the governing design code.
17-4PH vs 15-5PH, 410, 304 and 316L
| Grade | Main Strength | Main Limitation | Typical Selection Reason |
|---|---|---|---|
| 17-4PH | Very high strength after aging with useful corrosion resistance | Less formable than austenitic grades | High-strength shafts, valves, aerospace parts and machined components |
| 15-5PH | High strength with good transverse toughness | Often less widely available | High-reliability aerospace and precision parts |
| 410 | Hardenable and comparatively economical | Lower corrosion/toughness balance than 17-4PH | General hardenable stainless components |
| 304 | Excellent formability and weldability | Much lower strength without cold work | General fabrication and corrosion-resistant equipment |
| 316L | Better chloride resistance and easy fabrication | Much lower strength than aged 17-4PH | Wet chemical, food and chloride-exposed equipment |
17-4PH Stainless Steel Supply Forms
XRTGSteel can source 17-4PH stainless steel in several product forms through mill and processing routes. Availability should be confirmed against the required specification, size, heat-treatment condition and quantity rather than assumed from a generic grade list.
| Product Form | Relevant XRTGSteel Page | Important RFQ Information |
|---|---|---|
| Round / Flat Bar | Stainless Steel Bar | Diameter or section, length, standard, condition, surface and testing. |
| Sheet / Plate | Stainless Steel Sheet / Plate | Thickness, width, length, standard, condition and surface. |
| Coil / Strip | Stainless Steel Coil / Stainless Steel Strip | Thickness, width, coil weight, edge, condition and tolerance. |
| Forging / Custom Blank | Project-specific sourcing | Drawing, ASTM/AMS requirement, condition, machining allowance and NDT. |
| Pipe / Tube | Stainless Steel Pipe / Tube | Confirm availability, manufacturing route, OD, wall, length and governing specification. |
Processing, Inspection and Documentation
Processing and inspection requirements should be defined before quotation whenever they affect final mechanical properties or dimensional acceptance.
| Requirement | Typical Order Consideration |
|---|---|
| Saw Cutting / Cut-to-Length | Finished length, machining allowance and dimensional tolerance. |
| Laser Cutting | Drawing, thickness, edge condition and downstream machining requirement. |
| Slitting | Strip width, width tolerance, edge requirement and coil condition. |
| Surface Finishing | Ground, polished, peeled, turned or other specified finish. |
| Heat Treatment | Condition A, H900, H925, H1025, H1075, H1100, H1150 or project-specific requirement. |
| Mechanical Testing | Tensile, yield, elongation, hardness and impact requirements where applicable. |
| NDT / Verification | PMI, UT, dimensional inspection or third-party inspection when specified. |
| Documentation | MTC, heat-treatment records, inspection reports and packing documents as required by the order. |
XRTGSteel's stainless steel processing services cover the main cutting, finishing and export preparation routes used for project orders.
How to Specify 17-4PH on an RFQ or Purchase Order
A useful 17-4PH inquiry should identify more than the grade name. The following information reduces technical clarification and quotation delays.
- Material: 17-4PH / UNS S17400 / Type 630 / EN 1.4542 as required.
- Product standard: ASTM A564, ASTM A693, ASTM A705, AMS 5604, AMS 5643 or project specification.
- Product form: bar, forging, sheet, plate, strip, coil, tube or custom blank.
- Dimensions: diameter, thickness, width, length and dimensional tolerance.
- Heat-treatment condition: Condition A, H900, H925, H1025, H1075, H1100 or H1150.
- Quantity: pieces, kilograms, tons or coil quantity.
- Testing: MTC, hardness, tensile, impact, PMI, UT or third-party inspection where required.
- Processing: saw cutting, machining allowance, laser cutting, slitting, grinding or polishing.
- Application: service environment, temperature and required mechanical-property level.
- Delivery: destination port, Incoterm and required packing method.
For critical parts, send the drawing and governing specification together with the RFQ. This is more reliable than selecting material solely from a generic grade-comparison table.
FAQ About 17-4PH Stainless Steel
Is 17-4PH the same as 630 stainless steel?
17-4PH is commonly identified as Type 630 / AISI 630 and UNS S17400. EN 1.4542 and SUS630 are commonly referenced international designations. The governing product specification must still be checked before purchase.
What does H900 mean in 17-4PH?
H900 is a precipitation-aging condition using a nominal aging temperature of 900°F / 482°C. It is commonly selected when very high strength and hardness are required.
What is the difference between H900 and H1150?
H900 generally provides higher strength and hardness. H1150 uses a higher aging temperature and generally provides lower strength with improved ductility and toughness. The correct condition depends on the design requirement and service environment.
Is 17-4PH magnetic?
Yes. 17-4PH is a martensitic precipitation-hardening stainless steel and is magnetic in its common solution-treated and aged conditions.
Is 17-4PH more corrosion resistant than 316L?
Not generally in severe chloride exposure. 17-4PH is selected primarily for its high-strength/corrosion-resistance balance, while 316L is often preferred where chloride corrosion resistance and fabrication are more important than very high heat-treated strength.
What should be included on a 17-4PH material certificate?
The required certificate content depends on the governing specification, but buyers commonly verify heat number, chemistry, heat-treatment condition, mechanical test results and applicable product standard. Additional NDT or inspection documentation should be specified in the purchase order.
Request a 17-4PH Stainless Steel Quote
Send the required material designation, product form, size, specification, heat-treatment condition, quantity, testing requirement and destination. For machined, forged, aerospace, valve, pump or other critical components, include the drawing and acceptance requirements with the inquiry.
XRTGSteel can then confirm the appropriate sourcing route, available product form, processing requirement, documentation and packing before quotation.
Contact XRTGSteel